Recycling plastics from end-of-life vehicles (ELVs) is an important part of improving resource recovery and supporting more circular use of plastics. Among the available technologies, pyrolysis — thermal decomposition of polymers at elevated temperatures without oxygen — has emerged as a promising route for recovering fuels and chemicals. A recent study examined how plastics recovered directly from vehicle components behave during thermal and catalytic pyrolysis, testing a low-cost iron-pillared clay catalyst against purely thermal processing.
Earlier work has shown that pyrolysis can convert common automotive plastics such as low-density polyethylene (LDPE), high-density polyethylene (HDPE), and polypropylene (PP) into valuable hydrocarbons at relatively high yields. Much of that research, however, focused on automotive shredder residue, a heterogeneous mixture of plastics, metals, textiles, and other materials. That leaves less information about plastics recovered directly from components such as dashboards, bumpers, and headlamps. Automotive plastic waste (APW) can also contain mineral fillers, flame retardants, fiberglass, and other additives that affect degradation behavior and product composition.
Catalyst selection and feedstock
Catalysts can improve pyrolysis efficiency by accelerating reactions, altering product distributions, and potentially reducing the required temperature or residence time. Commercial zeolites have been widely studied, but lower-cost clay-based alternatives are drawing increasing interest. Among them, pillared clays modified with metals such as iron, titanium, or zirconium have shown potential to increase liquid yields and influence the formation of fuel-range hydrocarbons. Iron-modified clays are particularly attractive because they may improve oil production without relying on more expensive commercial catalysts.
In the study, the researchers characterized plastics recovered directly from ELVs before pyrolysis. The feedstock contained acrylonitrile butadiene styrene (ABS), HDPE, LDPE, PP, polystyrene (PS), and fiberglass, along with substantial volatile and ash fractions. Front and rear bumpers accounted for 86.6% of the sample by weight, and fiberglass used to reinforce automotive components contributed to the relatively high ash content. Rather than using bentonite clay in its original form, the team modified it through iron pillaring, a process that introduces iron species into the clay structure and changes characteristics such as surface acidity and pore structure.
Yield rises, composition shifts less
The team compared thermal and catalytic pyrolysis across temperatures ranging from roughly 350°C to 521°C and catalyst loadings of about 6% to 34% by weight, using a statistical experimental design to evaluate the interaction between temperature and catalyst concentration.
The catalyst strongly affected liquid yield. Catalytic pyrolysis produced an average oil yield of approximately 68%, compared with 41% for thermal pyrolysis alone. The highest oil yield, 78.6%, was achieved at about 416°C with a catalyst loading of roughly 24%.
However, the catalyst had much less influence on the composition of the resulting oil. Thermal and catalytic pyrolysis produced similar proportions of hydrocarbons within the C8-C24 range associated with gasoline- and diesel-range compounds. In other words, the catalyst helped convert more of the plastic feedstock into liquid product but did not substantially shift that liquid toward a higher proportion of diesel-range molecules. Temperature had a greater effect on product composition: lower pyrolysis temperatures favored diesel-range organics, while temperatures above 450°C produced a heavier, waxier oil.
Diesel-range promise, with caveats
The resulting pyrolysis oil showed several properties comparable to those of commercial diesel. The researchers reported a calorific value of 49.85 MJ/kg, a flash point of 113°C, and total aromatics of 3.55% by area — values within or comparable to ranges specified for conventional fuels. Branched heptenes and heptanes dominated the oil, compounds also identified in previous studies of polypropylene and automotive-plastic pyrolysis.
Not all properties met diesel specifications, though. Both density and viscosity exceeded the limits typically specified for diesel fuel, which the researchers attributed partly to heavier, long-chain hydrocarbon fractions remaining in the pyrolysis oil. Additional processing could therefore be required before the oil could be used as a diesel-range fuel. The researchers suggested approaches such as distillation and centrifugation, as well as optimizing reaction conditions through lower temperatures and longer residence times, to reduce heavier fractions and improve fuel properties.
Development still needed
The study positions pyrolysis as a technically promising route for recovering value from automotive plastics, while also highlighting the additional development required before the process can move toward broader commercial application. Future work could investigate different iron concentrations in the catalyst, improve reactor designs and heat transfer, and combine pyrolysis with downstream distillation to separate gasoline- and diesel-range fractions.
Improved collection and sorting of automotive plastics will also be important. Without systematic removal and classification of plastic components from end-of-life vehicles, reliable data on the volume and composition of available automotive plastic waste remain limited. Better information on these waste streams would help researchers and recyclers assess feedstock availability and plan potential industrial-scale pyrolysis operations.