Natural Pigments Compound into PLA and PBS, but Light Stability Caps Their Use

Spirulina, curcumin, beetroot and chlorophyllin masterbatches ran on conventional twin-screw equipment with modest effects on melt flow and mechanical performance, while 50 hours of xenon exposure left most formulations visibly changed.

A study titled "Sustainability in the Development of Natural Pigment-Based Colour Masterbatches and Their Application in Biopolymers" has examined whether four commercial natural colorants can pass through industrial melt processing in biodegradable polyesters without losing colour, flow behaviour or mechanical performance. The pigments — blue spirulina, yellow curcumin, red beetroot and green chlorophyllin — were compounded into polylactic acid (PLA) and polybutylene succinate (PBS). Most formulations ran on conventional equipment, but colour retention at temperature and lightfastness defined the practical limits.

The researchers produced colour masterbatches by twin-screw extrusion, adding titanium dioxide, calcium carbonate and stearic acid to support UV protection, dispersion and processing. The masterbatches were then diluted into the matching polymer matrix at 2, 4 and 6 wt%, and test specimens were produced by injection moulding.

A narrow thermal window

Heat is the central constraint, because the organic pigments start to degrade at lower temperatures than the polymers carrying them. Thermogravimetric analysis placed degradation onset at approximately 229 °C for spirulina, 244 °C for curcumin, 258 °C for chlorophyllin and 267 °C for beetroot, while PLA and PBS degrade at considerably higher temperatures. The team therefore set extrusion profiles that melted each polymer while keeping pigment exposure short: 145 °C for PBS and 190 °C for PLA, with the twin-screw extruder running at 65 rpm and a feed rate of 2 kg/h.

That window suited most pigment–polymer pairs with one clear exception. During PLA processing spirulina lost its blue colour, so a blue PLA masterbatch could not be made; in PBS, whose lower processing temperature was gentler, enough pigment survived for successful compounding. The outcome indicates that pigment compatibility depends strongly on what a given matrix requires thermally, not on the colorant alone.

Modest shifts in flow and mechanics

Rheology moved only slightly. Neat PLA showed a melt flow rate of about 50 g/10 min, and the natural-pigment masterbatches stayed close to that figure; PBS responded in a similar way with a minor reduction. The small decline points to a modest rise in melt viscosity. For compounders the point is practical: a colour system that forced major changes to screw design, pressure settings or moulding conditions would offer little value, and here conventional twin-screw compounding and injection moulding handled most formulations.

Mechanical baselines were largely preserved across the 2 to 6 wt% range. PLA started from a Young's modulus of about 1710 MPa and tensile strength of 65.6 MPa, PBS from roughly 392 MPa and 34.5 MPa, and the coloured formulations stayed close to those values. Impact strength also remained in a comparable range, although individual pigments introduced some variation.

Light stability emerges as the main barrier

Successful extrusion did not translate into durable colour. After 50 hours of xenon-lamp exposure, most formulations showed a colour difference above ΔE* = 2, a level treated as visually perceptible. The exception was a PLA formulation containing 2 wt% green chlorophyllin masterbatch, which showed the highest photostability. The study points to UV stability as the largest obstacle to broader use, noting that packaging, consumer products, agricultural parts and outdoor applications may need additional stabilization, protective coatings or pigment modification before natural colours can match conventional systems over long service lives.

Lower footprint under the study's assumptions

The environmental comparison favoured the natural route on the study's own assumptions: one kilogram of curcumin pigment was associated with about 0.04 kg CO2-eq, against 18.65 kg CO2-eq for the inorganic green reference pigment. The natural-pigment masterbatches also consumed less electricity during extrusion and pelletizing.

The work concludes that further development is needed, particularly in lightfastness and thermal stability, but that several natural colorants can be compounded into PLA and PBS on conventional processing equipment with only limited changes in melt viscosity and mechanical performance.

MV

Mirela Varga

Mirela Varga evaluates polymer test reports, virgin and post-consumer recycled feedstock, lot variability, and supplier evidence for rubber and plastic products. Her coverage interprets ASTM D412 tension data, ISO 527 results, compression set, melt flow rate with test condition, and density without treating a single lot as a universal grade limit. She helps quality and reliability teams, sourcing managers, compound engineers, and packaging development managers compare documented evidence, verify scope-specific compliance, and decide whether to qualify, retest, or reject incoming material.